{"id":4788,"date":"2026-11-21T12:57:38","date_gmt":"2026-11-21T04:57:38","guid":{"rendered":"https:\/\/sanezenrubber.com\/?p=4788"},"modified":"2026-11-21T13:15:55","modified_gmt":"2026-11-21T05:15:55","slug":"nano-silica-alumina-alloy-particle-size-is-the-design-variable-not-the-quality-grade","status":"publish","type":"post","link":"https:\/\/sanezenrubber.com\/es\/technical-communication\/nano-silica-alumina-alloy-particle-size-is-the-design-variable-not-the-quality-grade\/4788\/","title":{"rendered":"Nano silica-alumina alloy: particle size is the design variable, not the quality grade"},"content":{"rendered":"<p class=\"wp-block-paragraph\"><strong>What this page answers<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">In filler marketing, smaller is presented as better. Twenty nanometres beats fifty, and fifty beats five hundred. That ranking is wrong as a design rule, and a tread compound is where it shows most clearly.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The material on this page has an average particle size of about 500 nanometres, against a D50 of 583 nanometres, which is roughly twenty five times the primary particle size of a precipitated silica. It cannot compete with silica as a reinforcing filler and it is not sold as one. What it can do is sit at the tread surface as a hard inorganic asperity and change friction, which is a different job that needs a different particle size.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">This page sets out the consequences of that size difference with the measured data: why 12.5 phr added on top of 80 phr of silica leaves hardness unchanged, why substituting the same weight for silica takes five points of hardness away, and why the friction benefit shows up in a coefficient of friction test rather than in a modulus. It also reports the one result that stopped a project, which is shrinkage in a motorcycle tread.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Two numbers that decide what a filler can do<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A filler&#8217;s reinforcing effect depends on how much surface it presents to the polymer, and surface area per unit mass scales inversely with particle size. A 20 nm particle has twenty five times the specific surface of a 500 nm particle of the same density.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">That one relationship explains most of what follows.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td><strong>Particle size<\/strong><\/td><td><strong>Specific surface, relative<\/strong><\/td><td><strong>What the filler can do<\/strong><\/td><td><strong>Typical role<\/strong><\/td><\/tr><tr><td>20 to 30 nm<\/td><td>Muy alto<\/td><td>Reinforce strongly through a coupled interface<\/td><td>Precipitated silica, carbon black<\/td><\/tr><tr><td>100 to 300 nm<\/td><td>Alta<\/td><td>Reinforce moderately, carry a coupling reaction<\/td><td>Fine mineral fillers<\/td><\/tr><tr><td>About 500 nm<\/td><td>Moderado<\/td><td>Act at a surface rather than through the bulk<\/td><td>Friction, abrasion, wet grip<\/td><\/tr><tr><td>1 to 10 micrometres<\/td><td>Bajo<\/td><td>Fill volume and reduce cost<\/td><td>Kaolin, talc, calcium carbonate<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">The third row is where this material sits, and the row above it is where most nano fillers claim to be. An <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>alumina silicate filler for rubber<\/u><\/strong><\/a>&nbsp;at 500 nm does not have the surface to build the network that a 20 nm silica builds, and that is a limitation to be designed around rather than argued with.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>What the particle size distribution actually says<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The published figure for this material is an average particle size of about 500 nanometres. A laser diffraction measurement on a production sample gives the full distribution, and the distribution is more interesting than the average.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td><strong>Measurement<\/strong><\/td><td><strong>Valor<\/strong><\/td><\/tr><tr><td>D10<\/td><td>0.104 micrometre<\/td><\/tr><tr><td>D25<\/td><td>0.188 micrometre<\/td><\/tr><tr><td>D50<\/td><td>0.583 micrometre<\/td><\/tr><tr><td>D75<\/td><td>10.108 micrometres<\/td><\/tr><tr><td>D90<\/td><td>18.137 micrometres<\/td><\/tr><tr><td>D97<\/td><td>27.769 micrometres<\/td><\/tr><tr><td>Surface mean D(3,2)<\/td><td>0.288 micrometre<\/td><\/tr><tr><td>Volume mean D(4,3)<\/td><td>6.114 micrometres<\/td><\/tr><tr><td>Span<\/td><td>30.9<\/td><\/tr><tr><td>Specific surface, weight basis<\/td><td>20,834 m2\/kg, or 20.8 m2\/g<\/td><\/tr><tr><td>Coefficient of variation<\/td><td>138 percent<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<figure class=\"wp-block-image size-full\"><img alt=\"\" fetchpriority=\"high\" decoding=\"async\" width=\"494\" height=\"464\" src=\"https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/6150a283-636c-455f-af21-eaf371c9bab1.png.webp\" class=\"wp-image-4790\" srcset=\"https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/6150a283-636c-455f-af21-eaf371c9bab1.png.webp 494w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/6150a283-636c-455f-af21-eaf371c9bab1-300x282.png.webp 300w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/6150a283-636c-455f-af21-eaf371c9bab1-13x12.png.webp 13w\" sizes=\"(max-width: 494px) 100vw, 494px\" \/><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><em>Figure 1. The laser diffraction report behind the table. The curve is bimodal, with a fine population above 200 nm and a coarse one between 10 and 20 micrometres; the axis labels on the original report are in Chinese.<\/em><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Two things stand out, and both change how the material should be specified.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The first is that the distribution is bimodal. There is a fine fraction with a peak a little above 200 nanometres and a coarse fraction peaking in the ten to twenty micrometre region, with roughly half the volume below 10 micrometres and a quarter below 188 nanometres. The curve is not a single population with a tail; it is two.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The second is the surface area. At 20.8 m2\/g the material has between a tenth and a sixth of the specific surface of a precipitated silica, which typically sits between 120 and 200 m2\/g. That single number settles the argument about whether it can replace silica: at a tenth of the surface it cannot, and no dosage makes up the difference within the hardness budget.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>What is the difference between 20 nm silica and 500 nm alumina silicate<\/strong>&nbsp;is therefore not really a difference between two particle sizes. It is the difference between a material with 150 m2\/g of coupled surface and a material with 21 m2\/g arranged in two populations, one of which is not nano at all.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">That has a commercial consequence worth stating plainly. A customer who reads &#8220;500 nm&#8221; and then measures the D90 at 18 micrometres will question the data sheet. The D50 is 583 nanometres and it is correctly quoted; the volume mean D(4,3) is 6.1 micrometres, and both belong on the sheet. Publishing the distribution rather than the average would stop the conversation before it starts.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">En <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>particle size of a tread additive<\/u><\/strong><\/a>&nbsp;is therefore a specification item in its own right, alongside the chemistry. <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>Why does particle size matter in a tread compound<\/u><\/strong><\/a>&nbsp;is therefore not a question about quality. It is a question about which of the four roles the compound is short of, and a compound short of surface needs silica while a compound short of surface friction needs something coarser.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>What the material is, and where the bond forms<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The product is a hydrated aluminium silicate with aluminium and silicon distributed through the same particle. It is sold as a <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>nano silica alumina alloy<\/u><\/strong><\/a>, and the phrase describes the composition rather than the particle size. It is added at 10 to 30 phr in the first mixing stage, together with a silane.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The reaction that matters happens at temperature. X-ray photoelectron spectroscopy of a silica and silane system with and without the additive shows the aluminosilicate signal appearing once the batch passes about 165 C, and not at 120 C. A scanning electron micrograph at 20,000 times shows the same thing structurally: the outline of the original particle becomes a diffuse region of alumina or aluminosilicate as the batch heats.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Why does an Al-O-Si bond need 165 C<\/strong>&nbsp;is the practical question behind that measurement. The reaction is between the aluminium site and the silane, and it needs the thermal energy that only arrives above that temperature. It means the additive has to be in the batch during the hot part of the mix, with the silane, and not added at the end when the silane has already reacted.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Como <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>silane coupled mineral additive<\/u><\/strong><\/a>&nbsp;the material is therefore a co-reactant rather than a substitute. Nothing in the data suggests it replaces silane, and in all the trials below the silane level was held constant.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Trial one: added on top of 80 phr of silica<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">This is the standard test for an <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>additive for silica filled compound<\/u><\/strong><\/a>: the silica, the silane and the cure are held, and the additive is the single variable, so whatever moves is attributable to it.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td><strong>Material, phr<\/strong><\/td><td><strong>Blank<\/strong><\/td><td><strong>15 phr<\/strong><\/td><td><strong>12.5 phr<\/strong><\/td><\/tr><tr><td>SSBR<\/td><td>70<\/td><td>70<\/td><td>70<\/td><\/tr><tr><td>Butadiene rubber<\/td><td>30<\/td><td>30<\/td><td>30<\/td><\/tr><tr><td>Carbon black N234<\/td><td>5<\/td><td>5<\/td><td>5<\/td><\/tr><tr><td>S\u00edlice precipitada<\/td><td>80<\/td><td>80<\/td><td>80<\/td><\/tr><tr><td>Silane Si 75<\/td><td>6.8<\/td><td>6.8<\/td><td>6.8<\/td><\/tr><tr><td>Additives and cure system<\/td><td>30.2<\/td><td>30.2<\/td><td>30.2<\/td><\/tr><tr><td>Nano silica-alumina alloy<\/td><td>&#8211;<\/td><td>15<\/td><td>12.5<\/td><\/tr><tr><td>Total<\/td><td>219.2<\/td><td>234.2<\/td><td>231.7<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td><strong>Propiedad<\/strong><\/td><td><strong>Blank<\/strong><\/td><td><strong>15 phr<\/strong><\/td><td><strong>12.5 phr<\/strong><\/td><\/tr><tr><td>Viscosidad Mooney<\/td><td>59.8<\/td><td>55.9<\/td><td>55.5<\/td><\/tr><tr><td>MH, dN.m<\/td><td>14.05<\/td><td>14.59<\/td><td>15.06<\/td><\/tr><tr><td>t90, min<\/td><td>6.66<\/td><td>6.27<\/td><td>6.04<\/td><\/tr><tr><td>\u00cdtems de prueba<\/td><td>64.2<\/td><td>64.8<\/td><td>64.7<\/td><\/tr><tr><td>Resistencia a la tracci\u00f3n, MPa<\/td><td>24.8<\/td><td>27.9<\/td><td>25.3<\/td><\/tr><tr><td>Elongation at break, percent<\/td><td>420.6<\/td><td>433.4<\/td><td>436.0<\/td><\/tr><tr><td>Modulus at 100 percent, MPa<\/td><td>3.5<\/td><td>3.9<\/td><td>4.2<\/td><\/tr><tr><td>Modulus at 300 percent, MPa<\/td><td>15.5<\/td><td>17.4<\/td><td>17.8<\/td><\/tr><tr><td>Tear strength, kN\/m<\/td><td>18.1<\/td><td>18.0<\/td><td>21.9<\/td><\/tr><tr><td>DIN abrasion loss, cm3<\/td><td>0.163<\/td><td>0.156<\/td><td>0.154<\/td><\/tr><tr><td>tan delta at 0 C<\/td><td>0.303<\/td><td>0.315<\/td><td>0.328<\/td><\/tr><tr><td>tan delta at 60 C<\/td><td>0.106<\/td><td>0.097<\/td><td>0.095<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Why hardness did not move, and what it tells you<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Fifteen phr of a mineral filler added to a compound already carrying 80 phr of silica raised hardness by 0.6 of a Shore A point. Two phr less raised it by 0.5. By any normal filler arithmetic that is impossible: a mineral at 2.5 g\/cm3 displacing nothing should add several points.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Why does hardness not change when adding a coarse filler<\/strong>&nbsp;has a specific answer in this system. Hardness in a filled elastomer is set by the volume of filler and by the strength of the filler network, and a coarse particle contributes volume while contributing little network. The compound also shows the network relaxing: Mooney viscosity falls and MH rises, which is not the pattern of a filler being loaded, but the pattern of one network being replaced by a denser chemical one.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">That is the first consequence of the coarse particle and it is useful commercially. An additive that raises modulus and tear without raising hardness lets a formulator change performance inside a fixed hardness window, which is where most tread specifications live.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The modulus result is the exception that proves the rule. M100 rose 20 percent and M300 rose 15 percent at 12.5 phr. The coarse particle does not build a network, but it does concentrate stress at high strain, which stiffens the compound in the region where the polymer is already stretched. A <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>tread surface friction additive<\/u><\/strong><\/a>&nbsp;that stiffens at 300 percent elongation while leaving hardness alone is a specific combination.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Trial two: substituted for 11 phr of silica<\/strong><\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td><strong>Propiedad<\/strong><\/td><td><strong>Blank<\/strong><\/td><td><strong>Alloy 11 phr<\/strong><\/td><\/tr><tr><td>Silica, phr<\/td><td>70<\/td><td>59<\/td><\/tr><tr><td>Total compound, phr<\/td><td>216.3<\/td><td>205.3<\/td><\/tr><tr><td>Mooney ML(1+4)<\/td><td>74.18<\/td><td>65.26<\/td><\/tr><tr><td>Scorch at 130 C, min<\/td><td>37.4<\/td><td>47.6<\/td><\/tr><tr><td>T90, min<\/td><td>24.6<\/td><td>26.6<\/td><\/tr><tr><td>\u00cdtems de prueba<\/td><td>63.4<\/td><td>58.44<\/td><\/tr><tr><td>Modulus at 300 percent, MPa<\/td><td>8.68<\/td><td>8.52<\/td><\/tr><tr><td>Resistencia a la tracci\u00f3n, MPa<\/td><td>21.6<\/td><td>23.8<\/td><\/tr><tr><td>Elongation at break, percent<\/td><td>600<\/td><td>653<\/td><\/tr><tr><td>Resilience, percent<\/td><td>49<\/td><td>55<\/td><\/tr><tr><td>tan delta at 0 C<\/td><td>0.284<\/td><td>0.322<\/td><\/tr><tr><td>tan delta at 60 C<\/td><td>0.133<\/td><td>0.120<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Here 11 phr of silica was removed and 11 phr of the alloy added. Hardness fell from 63.4 to 58.44, five points.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to keep hardness when replacing silica with a mineral<\/strong>&nbsp;is the question this trial answers by showing what happens when you do not try. You removed 11 phr of a 20 nm reinforcing filler and replaced it with 11 phr of a 500 nm particle, so you removed surface area and network and replaced them with volume. Hardness follows the network, and the network was reduced.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The dynamic result is better in this trial than in the first: the loss factor at 0 C rose 13.4 percent and at 60 C fell 9.8 percent. Some of that gain is the softer compound rather than the additive, which is the trap in a substitution trial: two things changed, and the hardness drop is one of them.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The scorch result is worth a line. It moved from 37.4 to 47.6 minutes, a 27 percent longer safety window, which is the behaviour of a surface that does not hold accelerators. A <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>mineral additive with Al-O-Si bond<\/u><\/strong><\/a>&nbsp;formation takes the silane into a different reaction, and the cure sees less of it.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>The friction result, which is the reason the particle size is 500 nm<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The most direct evidence for the surface mechanism is not a tread property at all but a tribology test on the compound surface.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td><strong>Measurement<\/strong><\/td><td><strong>Blank<\/strong><\/td><td><strong>With the alloy<\/strong><\/td><\/tr><tr><td>Coefficient of friction<\/td><td>reference<\/td><td>17.3 percent higher<\/td><\/tr><tr><td>Variation of friction with sliding speed<\/td><td>larger<\/td><td>smaller<\/td><\/tr><tr><td>Surface roughness after the friction test<\/td><td>rougher<\/td><td>finer<\/td><\/tr><tr><td>DIN abrasion loss, cm3<\/td><td>0.163<\/td><td>0.154<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">An <strong>inorganic particle for wet friction<\/strong>&nbsp;has to do two things at once: stay at the surface, and be hard enough that its contact with the road does not flatten with the rubber around it. Three things changed together in this test, and they are consistent with each other. The coefficient of friction rose 17.3 percent, which is the <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>additive to improve coefficient of friction<\/u><\/strong><\/a>&nbsp;claim in its most literal form. The friction became less dependent on sliding speed, which is what a hard inorganic asperity in contact with a counter-surface would do, because the contact is more mechanical and less viscoelastic. And the surface after the test was smoother rather than rougher, which is the opposite of what abrasive wear usually leaves.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to measure tread friction in the laboratory<\/strong>&nbsp;is the question that decides whether a claim like this is usable. A coefficient of friction measured against a laboratory counter-surface is not a wet braking result, and it should be treated as a screening measurement that supports a mechanism. <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>Why does surface roughness matter for wet grip<\/u><\/strong><\/a>&nbsp;follows from the same logic: a tread grips a wet road through a combination of adhesion and hysteresis, and a surface that stays smoother under sliding keeps a more uniform contact patch than one that is torn up.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>What is the optimum particle size for wet grip<\/strong>&nbsp;cannot be answered from one material. What this data supports is narrower and more useful: a particle large enough to stand proud of a water film and hard enough not to deform with the rubber has a friction benefit that a 20 nm particle does not, and 500 nm is in that range.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>The dynamic result, and the dosage that beats the higher one<\/strong><\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td><strong>Measurement<\/strong><\/td><td><strong>Blank<\/strong><\/td><td><strong>15 phr<\/strong><\/td><td><strong>12.5 phr<\/strong><\/td><\/tr><tr><td>tan delta at 0 C<\/td><td>0.303<\/td><td>0.315<\/td><td>0.328<\/td><\/tr><tr><td>Change at 0 C<\/td><td>&#8211;<\/td><td>+4.0 percent<\/td><td>+8.3 percent<\/td><\/tr><tr><td>tan delta at 60 C<\/td><td>0.106<\/td><td>0.097<\/td><td>0.095<\/td><\/tr><tr><td>Change at 60 C<\/td><td>&#8211;<\/td><td>-8.5 percent<\/td><td>-10.4 percent<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">Twelve and a half phr beat fifteen on both ends of the curve. As a <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>wet grip additive for tire tread<\/u><\/strong><u>&nbsp;y un<\/u> <strong><u>rolling resistance reduction additive<\/u><\/strong><\/a>&nbsp;the lower dosage was better on both counts, which means the response is not monotonic.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to compare two dosages of a mineral additive<\/strong>&nbsp;should therefore always include a point below the expected optimum. The reason the curve turns over is plausible and not proven: at higher loading the particles start to contact each other, the surface becomes dominated by the mineral rather than by the polymer, and the hysteretic contribution that produces grip at 0 C falls away. Whatever the cause, a single point trial can land on either side of the peak and give the wrong answer.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to reduce rolling resistance without losing grip<\/strong>&nbsp;is the question this data answers most completely: at 12.5 phr, rolling resistance improved 10.4 percent while wet grip improved 8.3 percent, in the same compound, with no change to the polymer or the silane.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>The result that stopped a project<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A high performance motorcycle tread was run with 10, 12.5 and 17.5 phr, with a fixed 4 phr of a second additive.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td><strong>Propiedad<\/strong><\/td><td><strong>Original<\/strong><\/td><td><strong>10 phr<\/strong><\/td><td><strong>12.5 phr<\/strong><\/td><td><strong>17.5 phr<\/strong><\/td><\/tr><tr><td>TC90, seconds<\/td><td>98<\/td><td>64<\/td><td>64<\/td><td>60<\/td><\/tr><tr><td>Hardness, JIS A<\/td><td>55<\/td><td>52<\/td><td>52<\/td><td>55<\/td><\/tr><tr><td>Resistencia a la tracci\u00f3n, MPa<\/td><td>16.5<\/td><td>16.5<\/td><td>14.8<\/td><td>15.7<\/td><\/tr><tr><td>Elongation at break, percent<\/td><td>471<\/td><td>453<\/td><td>426<\/td><td>419<\/td><\/tr><tr><td>Stress at 300 percent, MPa<\/td><td>8.6<\/td><td>9.5<\/td><td>8.9<\/td><td>9.6<\/td><\/tr><tr><td>Right angle tear, kN\/m<\/td><td>43.48<\/td><td>44.83<\/td><td>42.88<\/td><td>46.4<\/td><\/tr><tr><td>Trouser tear, kN\/m<\/td><td>15.5<\/td><td>15.8<\/td><td>13.7<\/td><td>19.2<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">All three dosages produced excessive compound shrinkage, which made the compound difficult to use in the application, and the source recommends the lowest dosage on that basis rather than on any of the properties.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Why did the motorcycle tread shrink<\/strong>&nbsp;is a question about thermal expansion and relaxation rather than about reinforcement. A mineral phase with a different expansion coefficient from the polymer changes how much the extruded profile moves as it cools, and at 10 to 17.5 phr that change is large enough to take the tread out of the die&#8217;s tolerance. It is a production constraint, and it is the kind of constraint that a properties table never shows.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to add a mineral additive in the first mixing stage<\/strong>&nbsp;matters here too, because dispersion affects shrinkage. A poorly dispersed mineral produces local concentrations that shrink differently from the bulk, and the profile distorts unevenly rather than uniformly.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Dosage, and how to set it<\/strong><\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td><strong>Art\u00edculo<\/strong><\/td><td><strong>Recommendation<\/strong><\/td><\/tr><tr><td>General dosage range<\/td><td>10 to 30 phr<\/td><\/tr><tr><td>Addition point<\/td><td>First mixing stage, with the silane<\/td><\/tr><tr><td>Dosage used as an additive<\/td><td>12.5 phr, which beat 15 phr on both loss factors<\/td><\/tr><tr><td>Dosage used as a silica replacement<\/td><td>11 phr, with a five point hardness loss<\/td><\/tr><tr><td>Practical limit where shrinkage matters<\/td><td>10 phr<\/td><\/tr><tr><td>Batch temperature needed for the bond<\/td><td>above 165 C during mixing<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Tread compound additive dosage<\/strong>&nbsp;has three defensible answers depending on the intent, and the table gives all three rather than one. The mistake is to read the 10 to 30 phr range as a recommendation and start at 20, which is above the dynamic peak and above the shrinkage limit at the same time.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Como <strong>abrasion resistance additive for tread<\/strong>&nbsp;compounds the effect is real and modest, and it does not come from hardness. <a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u>How to improve DIN abrasion with a mineral additive<\/u><\/strong><\/a>&nbsp;is the one property where the two dosages were close: 0.156 at 15 phr and 0.154 at 12.5 phr, against 0.163 for the blank. An abrasion index of 106 is a modest gain and it comes from the same interface improvement, not from a harder compound, because hardness did not move.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Where this belongs, and where it does not<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The particle size argument gives a clear boundary, and it is worth drawing it before a customer spends a trial.<\/p>\n\n\n\n<figure class=\"wp-block-table\"><table class=\"has-fixed-layout\"><tbody><tr><td><strong>Situation<\/strong><\/td><td><strong>What the data supports<\/strong><\/td><td><strong>What to watch<\/strong><\/td><\/tr><tr><td>Silica tread short of grip at the surface<\/td><td>Added at 12.5 phr, wet grip up 8.3 percent and rolling resistance down 10.4 percent<\/td><td>Test the dosage peak; 15 phr was worse<\/td><\/tr><tr><td>Silica tread short of bulk hardness or modulus<\/td><td>Not the right tool<\/td><td>It adds little network, so hardness will not move<\/td><\/tr><tr><td>Compound where silica can be displaced for cost<\/td><td>Possible at 11 phr, but check hardness first<\/td><td>Five points of hardness lost at equal weight<\/td><\/tr><tr><td>Process with a tight shrinkage tolerance<\/td><td>10 phr is the practical limit<\/td><td>Shrinkage stopped a motorcycle project at all three dosages<\/td><\/tr><tr><td>Mixing line that cannot reach 165 C<\/td><td>Not suitable<\/td><td>The bond does not form and the additive is inert<\/td><\/tr><tr><td>Compound with no silane<\/td><td>Not suitable<\/td><td>The bond needs the silane as a co-reactant<\/td><\/tr><\/tbody><\/table><\/figure>\n\n\n\n<p class=\"wp-block-paragraph\">The fourth and fifth rows are the ones that are usually discovered too late. Shrinkage is a die and cooling problem that shows up after the properties have been signed off, and a mixing line that peaks at 150 C will produce a compound that contains the additive and none of the chemistry.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Three measurements, and what each one can carry<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Any claim about a tread additive ends up resting on one of three measurements, and they are not equally strong.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The loss factor from a DMA temperature sweep is the standard proxy for rolling resistance and wet grip, and it is a good one because the tyre industry has calibrated it over decades. It is still a proxy, and it moves with strain amplitude, so the conditions have to be quoted with the number.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">DIN abrasion loss is a laboratory wear test on a small specimen against a rotating drum. It correlates with tread wear well enough to be used as a screening test, and it says nothing about the mechanisms that cause field wear, such as cutting and chipping on a rough surface.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">A coefficient of friction measured against a laboratory counter-surface is the weakest of the three as a performance predictor, and the most direct evidence of a surface mechanism. A 17.3 percent increase in a laboratory coefficient of friction should not be translated into a wet braking distance, and it does establish that the surface changed.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">The honest hierarchy is that the DMA result is the one to argue a specification with, the abrasion result supports it, and the friction result explains why it happened.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>What the data does not support<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Four claims that a supplier in this category might make and this data does not.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">It does not support calling the material a silica replacement at equal weight. At equal weight the compound lost five points of hardness; at equal volume it would lose more, because the mineral is denser.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">It does not support a dosage above the peak. Fifteen phr was worse than 12.5 on both loss factors, and 17.5 phr in the motorcycle compound was worse than 10 on tensile and elongation.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">It does not support a claim about wet braking, only about laboratory loss factor and coefficient of friction. Those are the right screening measurements and they are not a tyre result.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">And it does not support use without silane. The bond needs the silane and needs the temperature, and a compound mixed cool or dosed without silane is a different experiment.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Preguntas frecuentes<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Why does particle size matter in a tread compound<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Because surface area per unit mass scales inversely with particle size, and the reinforcing network is built on surface. A 20 nm silica has about twenty five times the specific surface of a 500 nm particle, so it builds a network that the coarser particle cannot. The coarser particle still contributes volume and surface friction, which is a different job.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to improve wet friction with a mineral additive<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Put a hard, coarse inorganic particle at the surface and couple it to the rubber so it stays there. In this work the coefficient of friction rose 17.3 percent and became less dependent on sliding speed, and the loss factor at 0 C rose 8.3 percent at 12.5 phr. Wet friction is a surface property, so the particle has to be at the surface.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>What is the difference between 20 nm silica and 500 nm alumina silicate<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Surface area, and therefore role. Silica at 20 nm reinforces through a silane-coupled network and sets hardness. The alumina silicate at 500 nm has a fraction of that surface, so it adds little network and little hardness, but it is large enough to stand proud of a water film and hard enough not to deform with the rubber.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to raise the coefficient of friction of a tread compound<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Change the surface rather than the bulk. A compound at the same hardness can have very different friction depending on what is at the surface, and in this work 12.5 phr of a coarse mineral raised the coefficient of friction by 17.3 percent at unchanged hardness. Confirm with a wet test before translating it into a braking claim.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Why does hardness not change when adding a coarse filler<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Because hardness follows the filler network, and a coarse particle at 12.5 phr adds volume without adding much network. In the trial here, hardness moved from 64.2 to 64.7 while M100 rose 20 percent, so the compound stiffened where it was stretched without getting harder at low strain.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to keep hardness when replacing silica with a mineral<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Compensate, because you cannot avoid the loss. Removing 11 phr of 20 nm silica and adding 11 phr of 500 nm mineral took hardness from 63.4 to 58.44, and the compensation is less plasticiser or more reinforcing black, followed by a re-measurement of the dynamic properties.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Why does an Al-O-Si bond need 165 C<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Because the reaction between the aluminium site and the silane needs thermal energy that only becomes available above that temperature. XPS shows the aluminosilicate signal at 210 C and not at 120 C. Practically, the additive must be present during the hot part of the mix, which is why it goes in at the first stage.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to improve DIN abrasion with a mineral additive<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Improve the interface rather than the hardness. DIN loss fell from 0.163 to 0.154 cm3 at 12.5 phr, an index of 106, at unchanged hardness. That is a modest gain and it is consistent with better stress distribution at the filler-polymer boundary rather than with a stiffer compound.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to measure tread friction in the laboratory<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Measure a coefficient of friction against a defined counter-surface at controlled speed and load, and record how it varies with speed. In this work the friction rose 17.3 percent and its speed dependence fell. That is a screening measurement for a mechanism, not a wet braking result.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Why does surface roughness matter for wet grip<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Because a tread grips a wet road through contact area and hysteresis, and a surface that is torn up under sliding loses contact uniformity. In this work the surface after the friction test was finer than the blank&#8217;s, which is the opposite of abrasive wear and consistent with a harder phase carrying the contact.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to add a mineral additive in the first mixing stage<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Add it with the silica and the silane, and make sure the batch passes 165 C before dump. The bond forms above that temperature, so a cool mix leaves the mineral in the compound without the chemistry. Dispersion also matters for shrinkage, because local concentrations shrink differently from the bulk.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Why did the motorcycle tread shrink<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Because a mineral phase with a different thermal expansion coefficient from the polymer changes how much the extruded profile relaxes as it cools. At 10, 12.5 and 17.5 phr all three compounds shrank excessively, and the dosage was set at 10 phr on that basis rather than on properties.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to compare two dosages of a mineral additive<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Use three points and put one below the expected optimum, because the curve turns over. In this compound 12.5 phr beat 15 phr on both the 0 C and the 60 C loss factors, so a two point comparison at 15 and 20 would have concluded the additive does not work.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>What is the optimum particle size for wet grip<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">This data supports a range rather than a number. A particle large enough to stand proud of a water film and hard enough not to deform with the rubber showed a friction benefit; a 20 nm particle of the same chemistry would sit inside the polymer rather than at the surface. About 500 nm is in the working range.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>How to reduce rolling resistance without losing grip<\/strong><\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Move the dispersion and the surface state rather than the whole curve. At 12.5 phr the loss factor at 60 C fell 10.4 percent while the loss factor at 0 C rose 8.3 percent, in the same compound. Both improved because the particle changes where the energy is dissipated rather than how much of it there is.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Why Choose Us<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Choosing a functional filler supplier is not only about purchasing a mineral powder. It is about selecting a technical partner that understands polymer compounding, physical failure mechanisms, and long-term product performance. As a leading&nbsp;<a href=\"https:\/\/sanezenrubber.com\/es\/product\/\"><strong><u><strong>specialty functional filler and performance additives manufacturer<\/strong><\/u><\/strong><\/a>, we bring decades of compounding expertise to every customer collaboration.<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">SaneZenChem operates five manufacturing facilities specialising in:<br>\u2022 Rubber Compounds<br>\u2022 Silicone Rubber Compounds<br>\u2022 Specialty Functional Fillers<br>\u2022 Flame Retardants<br>\u2022 Polymer Performance Additives<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Because we formulate and manufacture rubber and silicone compounds ourselves, every specialty product we develop originates from solving real production challenges rather than laboratory concepts alone. This application-driven approach allows us to deliver practical solutions that create measurable improvements in customer products \u2013 from eliminating processing viscosity spikes and preventing micro cracking, to ensuring high dielectric strength in harsh electrical environments. Our unique dual position as both a direct compounder and a premier specialty functional filler manufacturer means we are uniquely equipped to support rubber, epoxy, and electrical insulation manufacturers in achieving longer service life, processing efficiency, and ultimate reliability.<\/p>\n\n\n\n<figure class=\"wp-block-image size-large is-resized\"><img decoding=\"async\" width=\"1024\" height=\"769\" data-src=\"https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/wpscbopfm-1024x769.jpg.webp\" alt=\"Sane Zen Group full range of products solution for rubber industry\" class=\"wp-image-4791 lazyload\" style=\"--smush-placeholder-width: 1024px; --smush-placeholder-aspect-ratio: 1024\/769;aspect-ratio:1.3304347826086957;width:612px;height:auto\" data-srcset=\"https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/wpscbopfm-1024x769.jpg.webp 1024w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/wpscbopfm-300x225.jpg.webp 300w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/wpscbopfm-768x577.jpg.webp 768w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/wpscbopfm-16x12.jpg.webp 16w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/wpscbopfm-500x376.jpg.webp 500w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/wpscbopfm-600x451.jpg.webp 600w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/wpscbopfm.jpg.webp 1206w\" data-sizes=\"(max-width: 1024px) 100vw, 1024px\" src=\"data:image\/svg+xml;base64,PHN2ZyB3aWR0aD0iMSIgaGVpZ2h0PSIxIiB4bWxucz0iaHR0cDovL3d3dy53My5vcmcvMjAwMC9zdmciPjwvc3ZnPg==\" \/><\/figure>\n\n\n\n<figure class=\"wp-block-image size-large is-resized\"><img alt=\"\" decoding=\"async\" width=\"1024\" height=\"772\" data-src=\"https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/asdasd-1024x772.png.webp\" class=\"wp-image-4792 lazyload\" style=\"--smush-placeholder-width: 1024px; --smush-placeholder-aspect-ratio: 1024\/772;aspect-ratio:1.327188940092166;width:576px;height:auto\" data-srcset=\"https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/asdasd-1024x772.png.webp 1024w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/asdasd-300x226.png.webp 300w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/asdasd-768x579.png.webp 768w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/asdasd-16x12.png.webp 16w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/asdasd-500x377.png.webp 500w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/asdasd-600x453.png.webp 600w, https:\/\/sanezenrubber.com\/wp-content\/smush-webp\/2026\/11\/asdasd.png.webp 1319w\" data-sizes=\"(max-width: 1024px) 100vw, 1024px\" src=\"data:image\/svg+xml;base64,PHN2ZyB3aWR0aD0iMSIgaGVpZ2h0PSIxIiB4bWxucz0iaHR0cDovL3d3dy53My5vcmcvMjAwMC9zdmciPjwvc3ZnPg==\" \/><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\">P\u00f3ngase en contacto con<\/h2>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Direcci\u00f3n de la planta:<\/strong><br>Camino Baishou, Distrito Norte de la Zona de Desarrollo Econ\u00f3mico de Xuan Zhou<br>Xuan Cheng City, Anhui Province, China<\/p>\n\n\n\n<p class=\"wp-block-paragraph\"><strong>Direcci\u00f3n Comercial:<\/strong><br>Room 503, Building 1, Huixin International Edifice, No. 150 Puhuitang Road, Xuhui District, Shanghai, China 200030<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Tel:&nbsp;+86 136 7164 1995<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">Correo electr\u00f3nico: yorichen@sanezen.com&nbsp;<\/p>\n\n\n\n<p class=\"wp-block-paragraph\">P\u00e1gina web:&nbsp;<a href=\"https:\/\/sanezenrubber.com\/es\/\"><u>www.sanezenrubber.com<\/u><\/a><\/p>","protected":false},"excerpt":{"rendered":"<p>What this page answers In filler marketing, smaller is presented as better. Twenty nanometres beats fifty, and fifty beats five hundred. That ranking is wrong as a design rule, and a tread compound is where it shows most clearly. The material on this page has an average particle size of about 500 nanometres, against a [&hellip;]<\/p>","protected":false},"author":1,"featured_media":4790,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"_seopress_robots_primary_cat":"","_seopress_titles_title":"","_seopress_titles_desc":"","_seopress_robots_index":"","footnotes":""},"categories":[1],"tags":[],"class_list":["post-4788","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-technical-communication"],"blocksy_meta":[],"acf":[],"_links":{"self":[{"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/posts\/4788","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/comments?post=4788"}],"version-history":[{"count":1,"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/posts\/4788\/revisions"}],"predecessor-version":[{"id":4795,"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/posts\/4788\/revisions\/4795"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/media\/4790"}],"wp:attachment":[{"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/media?parent=4788"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/categories?post=4788"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/sanezenrubber.com\/es\/wp-json\/wp\/v2\/tags?post=4788"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}